MPT-RI001DO MSLA Dusty Olive
User Guide
APPLYLABWORK PRINTING TIPS
Check
- Tank and LCD screen are clean
- Shake well (60 sec) before pouring
- Tank and platform are tightened properly
Contents
Exposure Setting Recommendation Chart
Printer | Layer Thickness (μm) | Bottom (Burn-In) Layers | Normal Layer Exposure Time (s) | Bottom Layer Exposure Time (s) | Rest Time After Retract (s) | Lifting Distance (mm) | Lifting Speed (mm/min) | Retract Speed (mm/min) |
Shuffle | 50 | 6 | 10 | 40 | 6 | 5 | 60 | 150 |
100 | 6 | 15 | 40 | 6 | 5 | 60 | 150 | |
Shuffle XL | 50 | 6 | 9 | 40 | 8 | 5 | 60 | 150 |
100 | 6 | 13 | 40 | 8 | 5 | 60 | 150 | |
Sonic | 50 | 6 | 2.5 | 25 | 6 | 5 | 60 | 150 |
100 | 6 | 4.5 | 25 | 6 | 5 | 60 | 150 | |
Sonic Mini | 50 | 6 | 4 | 25 | 6 | 5 | 60 | 150 |
100 | 6 | 6 | 25 | 6 | 5 | 60 | 150 | |
Sonic Mighty 4K | 50 | 6 | 3.6 | 30 | 8 | 5 | 60 | 150 |
100 | 6 | 5 | 30 | 8 | 5 | 60 | 150 | |
Sonic Mighty 8K | 50 | 6 | 3.8 | 30 | 8 | 5 | 60 | 150 |
100 | 6 | 5.2 | 30 | 8 | 5 | 60 | 150 | |
Elegoo Mars2 Pro | 50 | 6 | 2.6 | 25 | 6 | 5 | 60 | 150 |
100 | 6 | 4 | 25 | 6 | 5 | 60 | 150 | |
Elegoo Mars3 Ultra 4K | 50 | 6 | 3.1 | 25 | 6 | 5 | 60 | 150 |
100 | 6 | 4.2 | 25 | 6 | 5 | 60 | 150 | |
Elegoo Staurn S |
50 | 6 | 3.4 | 25 | 8 | 5 | 60 | 150 |
100 | 6 | 4.6 | 25 | 8 | 5 | 60 | 150 | |
Anycubic Photon MonoX | 50 | 6 | 1.7 | 25 | 8 | 5 | 1 (mm/s) | 2.5 (mm/s) |
100 | 6 | 2.4 | 25 | 8 | 5 | 1 (mm/s) | 2.5 (mm/s) |
Each printer is unique, light intensity varies from printer to printer, even within same model and make. Please adjust normal exposure time from above recommended settings ± 2 (± 0.2 ~ 0.5 for Mono LCD printer) for optimal results.
Sizing calibration, stl file: https://www.thingiverse.com/thing:1586206
Washing
Submerge print in clean IPA (95+% concentration) for up to 5 minutes, gently shake-off/blow-off excess IPA, set prints in shaded, airy place to dry before post-curing. Extended time in IPA causes deformation.
Post Curing
Curing Chamber | Temperature (℃) | Time (min) |
Form cure (Formlabs) | 60 | 60 |
Phrozen cure XL (Phrozen) | – | 60 |
Mercury x Cure (Elegoo) | – | 60 |
For optimal material performance, 405 nm light of total energy per unit area required: 18000 mJ/cm².
Example: light power or curing chamber: 5 mW/cm² (higher power per unit area shortens curing time), 18000 (mJ) / 5 (mW) / 60 (sec) = 60 mins of curing time.
Storage
- Keep resin in shaded environment; temperature between 15℃ and 26℃
- NOT accessible to children
- Filter used resin before storage
- To extend tank life, limit prolong storing resin in tank
Notes: Slight pigment settlement is normal. Gently mix remaining resin in resin tank with soft wiper for color evenness. Ensure there are no pigment settled on the resin tank bottom before start printing.